Color and materials: lab dips, metamerism, hand feel, lab tests, acceptance
The document defines how to approve color and fabric before sewing and how to accept a material lot: lab dips and color tolerance, metamerism, material hand feel, lab tests (shrinkage, pilling, colorfastness, breaking force) and an acceptance record with the decision “pass, fail, for decision”.
Why this document
The technologist, materials buyer and quality team read this when they approve color and accept a lot of fabric or leather. It matters because a mismatch found after cutting or sewing is expensive: the lot is scrapped or becomes a dispute with the supplier, and the season’s deadline cannot be recovered. A lab dip and color tolerance fix what counts as normal, lab tests expose hidden defects such as shrinkage and pilling, and rule-based acceptance gives grounds to reject a lot. Without them a claim rests on opinion.
At a glance
- What is this document and why is it needed?
- The document defines how to approve color and fabric before sewing and how to accept a material lot: lab dips and color tolerance, metamerism, material hand feel, lab tests (shrinkage, pilling, colorfastness, breaking force) and an acceptance record with the decision “pass, fail, for decision”.
- Who owns the document and how often is it rebuilt?
- Maintained by the technologist or materials manager with quality control; approved by the head of product; in practice for every material lot before cutting, with results kept in the style dossier and at the supplier.
- What mistakes are the most common?
- Color assessed under one light -> metamerism shows only at the customer -> assess under several lights and on the assembled item. Test requirements not written before ordering -> a dispute with the supplier and no basis for a claim -> requirements in the specification and contract. Cutting without a shrinkage correction -> finished items smaller than the stated size -> correction in cutting and consumption.
For whom
- Brand
- A brand sets the color standard and material specification (composition, density, test values) and accepts material before cutting; it owns compliance and consumption with shrinkage. A color library and fabric standards are used for its own palette.
- Retail
- A retailer buying finished goods does not accept materials; it requires test reports and certificates from the supplier, checks selectively (especially for private label) and claims on color and shrinkage under the contract. For private label it works as a brand.
What it consists of
1. Color: system, standard, lab dip
- Color is defined in a color system (Pantone, NCS, own palette) and a standard on fabric; a numeric value in Lab space (L, a, b) is used to measure differences.
- Brand: Lab dip: a dyed fabric sample sent by the dye house; the brand approves, corrects or rejects it; the delta E tolerance is set in advance and recorded in the dossier.
2. Metamerism and viewing conditions
- Metamerism: two colors match under one light and differ under another; assessment uses several light sources (daylight, store, warm), not just one.
- Different materials (cotton, polyester, trims) are dyed with different dyes, so color match of the product is checked on the assembled item, not on separate parts.
3. Hand feel and appearance
- Material feel: softness, stiffness, drape, weight, smoothness; assessed against a standard on a scale and recorded in words and a score.
- Appearance: fabric defects (streaks, pulls, shade variation within a roll), shade variation between rolls and dye lots.
4. Laboratory tests
- Shrinkage after washing lengthwise and widthwise, pilling, colorfastness (washing, dry and wet rubbing, perspiration, light), breaking force, seam strength, fibre composition, additional safety parameters for children and skin-contact products.
- For each test: method, number of samples, requirement (at least or at most), result, conclusion. Requirements are the brand specification, often stricter than the regulatory minimum.
5. Material acceptance record
- Lot identification (supplier, lot, dye lot, length, width), test results, color and appearance assessment, decision: pass, fail, for decision (with a condition such as cutting with a shrinkage allowance).
- Rules: a lot with at least one critical measure “fail” does not go to cutting until a decision; the decision is signed by the technologist and quality control.
6. Brand and retailer: who checks what
- Brand: The brand sets the color, the ΔE tolerance and test requirements and owns the reference; fabric and trims lots are accepted before cutting, and the pass/fail decision is signed by the technologist or quality manager.
- Retailer: For other brands the retailer checks finished goods by risk: an AQL sample at the DC, tests on kids, leather and whites, color match to the photo on the card; for a private label it acts as a brand.
- Brand: The material specification in the tech pack: composition, weight, shrinkage, fastness, tolerances; responsibility for regulation compliance lies with the manufacturer or importer, so test reports are kept per lot.
- Retailer: Requesting test reports and declarations from the supplier brand before receipt: validity, number, match to the lot; a missing document blocks receiving at the DC.
- Brand: Fabric supplier statistics: share of failed lots, reasons, time to correct; used when choosing factories and revising price.
- Retailer: Brand statistics: returns for material reasons (pilling, color bleed, shrinkage) by brand; grounds for a claim and for range review.
How to read the result and which decisions follow
- The batch fails 1 indicator (“Pilling, grade (1–5)”), the others pass; lengthwise shrinkage of 2.2% requires a cut of 102.2 m per 100 m of finished goods. Decision: batch acceptance goes by a set of indicators; one failed indicator blocks shipment to the warehouse until it is decided what to do with the batch.
- Brand: lab dip and metamerism are checked under several light sources and on the finished item; ΔE is set in the factory brief before sewing. Decision: do not approve a color from one photo and one illumination.
- Retailer: the distribution center does not accept materials but accepts finished goods with protocols and certificates; require a set of documents and a sample check from the brand, and for pilling and shrinkage complaints return the batch with the protocol.
- Brand: at ΔE of 0.71 against a tolerance of 1.00 the color margin is sufficient, but a change of dye batch raises the spread; fix the standard and tolerance in the contract.
- Retailer: composition and labeling requirements (fibre, care) apply to you as a seller; a composition mismatch between the card and the label creates a claim, not only a return.
Control checks
- Check: 8 indicators, 1 failed; shrinkage of 2.2% and 1.4% is below the 3.0% limit, ΔE 0.71 is below 1.00 (code).
- Brand: the test limits in the example are illustrative; take real requirements from the brief, the contract and current technical regulations (unverified).
- Retailer: the protocol must refer to your batch (batch number and date), not to a supplier sample.
- Brand: measure shrinkage by the method and washing mode stated on the label, otherwise the cutting calculation is not reproducible.
- Retailer: check the growth of claims after washing against batches; a repeating batch points to the material, not the client.
Brand and retailer: further differences
- Retailer: for private label you take on the brand functions in materials: the laboratory, tolerances and batch acceptance become your processes, not the supplier.
Where the data comes from
| Data source | Fields |
|---|---|
| Material specification and tech pack | Composition, density, width, test requirements, color tolerance |
| Laboratory reports | Test results, methods, sample count, date, laboratory |
| Dye house samples and standards | Lab dips, Lab measurement, dye lot, shade variation between rolls |
| Production and returns data | Actual shrinkage in cutting, fabric defects, pilling and fading complaints |
How to build it step by step
- Step 1. Set the color (system, fabric standard, Lab value) and the delta E tolerance in the dossier.
- Brand: Step 2. Request lab dips and assess them under several light sources and on the assembled item.
- Brand: Step 3. Measure Lab and compute delta E to the standard; decide: approve, correct or reject.
- Step 4. Write test requirements into the material specification before ordering fabric.
- Brand: Step 5. On receipt take samples from several rolls and send them for testing.
- Step 6. Assess shade variation between rolls and hand feel against the standard; record fabric defects.
- Step 7. Compare test results with requirements; mark pass or fail per measure.
- Step 8. Determine the lot decision; for shrinkage within tolerance, correct the cutting plan.
- Step 9. Complete the acceptance record and send the supplier a claim for non-conformity.
- Step 10. Keep supplier statistics: share of failed lots and causes; use them when choosing factories.
- Brand: Step 11. Brand: enter shrinkage corrections in patterns and keep color and hand-feel references at least until the next repeat buy of the basics range.
- Retailer: Step 12. Retailer: introduce risk-based incoming inspection at the DC (kids, leather, light colors) and keep a log of material-related return reasons by brand.
Formulas
| Measure | Formulas | Note |
|---|---|---|
| Brand: Shrinkage | Shrinkage, % = (size before washing - size after) / size before x 100 | Measured lengthwise and widthwise separately; the norm is set by the specification. |
| Brand: Cutting correction for shrinkage | Cut length = final length / (1 - shrinkage) | The same for width; for stretch fabrics shrinkage is checked after relaxation. |
| Brand: Color difference delta E | Delta E = sqrt((L2 - L1)^2 + (a2 - a1)^2 + (b2 - b1)^2) | The simplest form of difference in Lab; the tolerance is set by the brand and checked by eye under several lights. |
| Brand: Material consumption with shrinkage | Consumption = net x (1 + waste) x length shrinkage correction | The correction goes into the tech pack consumption. |
Formulas in notation
- Shrinkage
s = (L_before − L_after) / L_before × 100
Specimen size before and after washing by the test method.- Cutting length
L_cut = L_final / (1 − s)
L_final is the needed finished length; s is shrinkage as a fraction.- Color difference
ΔE = √((L₂ − L₁)² + (a₂ − a₁)² + (b₂ − b₁)²)
CIELAB coordinates of the standard and the sample; the ΔE tolerance is set by the brief.- Margin to requirement
m = (limit − value) / limit × 100 or (value − limit) / limit × 100
The first form for at most, the second for at least.
Worked example
Exercise: fabric lot acceptance from laboratory results
| Measure | Result | Requirement | Conclusion |
|---|---|---|---|
| Shrinkage after washing, lengthwise, % | 2.2 | at most 3.0 | pass |
| Shrinkage after washing, widthwise, % | 1.4 | at most 3.0 | pass |
| Pilling, grade (1–5) | 3.0 | at least 3.5 | fail |
| Colorfastness to washing, grade | 4.0 | at least 4.0 | pass |
| Colorfastness to wet rubbing, grade | 3.0 | at least 3.0 | pass |
| Breaking force, warp, N | 520 | at least 450 | pass |
| Breaking force, weft, N | 410 | at least 350 | pass |
| Color difference lab dip vs standard, delta E | 0.71 | at most 1.00 | pass |
Notional: 1 measures fail; the lot goes “for decision” with cutting suspended until the pilling issue is decided (options: replacing the fabric or accepting at a discount under the contract). Lengthwise shrinkage is 2.2%, widthwise 1.4%: for 100 cm of finished length cut 102.2 cm, a correction of 2.2% lengthwise and 1.4% widthwise. The lab dip delta E of 0.71 fits the tolerance of 1.0. Values are notional.
Figures
Data as a table
| Measure | Margin to requirement |
|---|---|
| Shrinkage after washing, lengthwise, % | 26.7 |
| Shrinkage after washing, widthwise, % | 53.3 |
| Pilling, grade (1–5) | −14.3 |
| Colorfastness to washing, grade | 0 |
| Colorfastness to wet rubbing, grade | 0 |
| Breaking force, warp, N | 15.6 |
| Breaking force, weft, N | 17.1 |
| Color difference lab dip vs standard, delta E | 29.3 |
Margin to the requirement in lab results. The margin as a percentage of the requirement: a negative value means the indicator failed (pilling).
Data as a table
| Measure | Length before washing |
|---|---|
| 0 | 100 |
| 1 | 101 |
| 2 | 102 |
| 3 | 103 |
| 4 | 104 |
| 5 | 105 |
| 6 | 106 |
Cutting length per 100 m of finished fabric by shrinkage. The greater the shrinkage, the more fabric is needed before washing: at shrinkage twice the norm the growth in length speeds up noticeably. Horizontal axis: lengthwise shrinkage, %.
Specifics by category
- Apparel
- Main tests: shrinkage after washing, knit pilling, colorfastness to rubbing and washing, shade variation between rolls. Working hints (assumptions, not norms): cotton shrinkage no more than 3% in length and width, ΔE up to 1.0 for a basic color and up to 1.5 for a fashion color. Shrinkage is entered into cutting as a correction: pattern × (1 + shrinkage); a 2% error on 100 cm gives a 2 cm deviation in the finished item, almost half a size in length.
- Footwear
- Materials: leather, nubuck, textile, synthetics; EVA, polyurethane or rubber soles. Tests by component: sole bond strength (peel), repeated flex (upper and sole cracks), colorfastness of leather to rubbing and sweat, water resistance, sole slip. A leather lot is uneven in thickness and tension, so several hides are assessed, not one sample. Defects are more often in the adhesive and sole than in the fabric; take methods and thresholds from your own specification (unverified, norms not checked).
- Accessories
- Materials: leather, faux leather, metal, plating, glass, stones, textile. Tests: coating resistance to tarnish and abrasion, hardware corrosion, strength of clasps and handles under load, shade variation of leather and hardware between lots; requirements for metal in skin contact are checked separately (unverified). Precious metals: fineness and weight, assay supervision; costume jewelry: alloy composition and coating. Leather hand-feel is judged against the previous lot reference.
- Kids
- For kids safety of composition and dyes under TR CU 007/2011 matters (biological and chemical safety; products for newborns and underwear for children under 1 year made of natural materials, except fillings, per the EEC text). Colorfastness to saliva and sweat, no small detachable parts, seams without irritation. Shrinkage is critical: with a 6 cm height run a 3-5% shrinkage on a toddler item eats a size, so pre-shrinking or an allowance is used. Lab-dips of bright colors are checked for dye migration.
- Men
- Basics: shirt and suit fabrics, wool, cotton, blends; shrinkage, crease resistance, elbow pilling and colorfastness are critical. Color: dark and neutral shades (blue, gray, black) show noticeable metamerism; a repeat order of a basic must match the previous one in ΔE, so the reference is kept for years. Hand-feel and drape are compared with the previous season reference. Less fashion means more standardization: acceptance methods and thresholds can stay constant.
- Women
- More bright and pastel colors, prints and thin fabrics (chiffon, knit): the lab-dip is harder, metamerism and roll-to-roll shade variation are more visible, and the ΔE tolerance is set for key colors. Thin and stretch fabrics are tested for stretch and recovery, snags, pilling and show-through. Hand-feel and drape strongly influence sales. Shrinkage and knit skew produce fit complaints; fashion trials run in short lots, so there are more lab-dips per unit of product.
Common mistakes
- Color assessed under one light -> metamerism shows only at the customer -> assess under several lights and on the assembled item.
- Test requirements not written before ordering -> a dispute with the supplier and no basis for a claim -> requirements in the specification and contract.
- Cutting without a shrinkage correction -> finished items smaller than the stated size -> correction in cutting and consumption.
- Testing one roll -> shade and property variation unseen -> samples from several rolls and dye lots.
- Lot decisions are not recorded -> the same problems recur -> an acceptance record and supplier statistics.
Russian specifics
- Light industry products are subject to conformity assessment under technical regulation TR CU 017/2011; measures and test methods are confirmed by reports and certificates. Rule: CU Commission decision 876 of 09.12.2011: TR CU 017/2011 on safety of light-industry products (Customs Union Commission Decision of 09.12.2011 No. 876).
- Children products are subject to TR CU 007/2011 with strict requirements on the safety of materials and dyes. Rule: CU Commission decision 797 of 23.09.2011: TR CU 007/2011 on safety of products for children and adolescents (Customs Union Commission Decision of 23.09.2011 No. 797).
- Care symbols follow international notation (GOST ISO 3758); composition and care must match the actual material properties confirmed by testing. Rule: GOST ISO 3758: GOST ISO 3758 (care labeling symbols for textiles).
- Brand: before release conformity is confirmed under the light-industry regulation and, for kids, under TR CU 007/2011; the document type (declaration or certificate) depends on the product group, check with a certification body (unverified).
- Retailer: sells only goods with a valid conformity document and correct labeling; responsibility for selling non-conforming goods also lies with the seller (details unverified).